Die Casting
What Porosity Is and Why It's the Core Metric
Porosity in vacuum die casting refers to the volume fraction of voids inside a casting formed by entrapped gas or shrinkage during solidification. It is not a cosmetic issue but a fundamental metric that determines whether a part is usable: castings with high porosity have lower tensile strength and worse thermal conductivity, and more critically, cannot withstand heat treatment or welding—entrapped gas expands during heat treatment and causes surface blistering, while gas pores become direct defect sources during welding.
High-pressure die casting itself is a process highly prone to gas entrapment. Molten metal fills the cavity at extremely high speed, and the air in the cavity is enveloped into the metal before it can escape, remaining inside as gas pores after solidification. The idea behind vacuum die casting is straightforward: evacuate the cavity to negative pressure before filling, reducing the total amount of gas available for entrapment.
Data Speaks: The Relationship Between Vacuum Level and Porosity
The reduction in porosity from improved vacuum level is quantifiable. In comparative experiments on AlSi9Cu3 alloy, porosity reached 8.5% under atmospheric pressure (1013 mbar), dropping to 3.7% when evacuated to 100 mbar. Another study on AlSi12Fe alloy showed that raising vacuum from 275 mbar to 72 mbar reduced porosity from 0.152% to 0.046%.
These numbers demonstrate two things. First, the improvement of vacuum die casting over atmospheric die casting is order-of-magnitude, not marginal optimization. Second, pushing vacuum below 100 mbar can further reduce porosity, but the benefit curve gradually flattens—which explains why the industry separates high vacuum from ultra-high vacuum in discussion.
The Threshold of High Vacuum and What It Buys
The industry generally draws the line for high vacuum die casting at 50–100 mbar (absolute pressure), with below 50 mbar counted as ultra-high vacuum; demanding applications such as integrated die casting require even below 30 mbar. Crossing this line matters not for the porosity number itself but because the casting gains new process possibilities: high vacuum die casting can control internal gas content at extremely low levels, making die castings suitable for heat treatment and welding.
This point is often underestimated. Ordinary die castings cannot simply undergo T6 heat treatment because internal gas pores expand and blister at high temperature. Low porosity opens up room for downstream processes, not just a few more megapascals on the strength table.
Judging Whether a Vacuum Die Casting Solution Is Credible
When looking at porosity claims, don't just look at the vacuum number a supplier quotes—ask three things. First, where and when the vacuum is measured; actual pressure inside the cavity can differ greatly from the reading at the vacuum pump end. Second, the corresponding alloy and part type; under different materials and wall thicknesses, the same vacuum level may not yield the same porosity. Third, whether there is metallographic or X-ray inspection data for the same batch to support the claim, rather than results from a single sample.
Porosity is the outcome metric of vacuum die casting quality, while the evacuation capability, sealing reliability, and valve response speed of the vacuum system are the causes. Understanding this causal relationship is what allows you to make judgments between quotes and samples.